Abstract
AbstractThe procedure for in situ TEM measurements of bonding strength (adhesion) between diamond and the metal matrix using a Hysitron PI 95 TEM Picoindenter holder for mechanical tests and Push-to-Pull devices was proposed. For tensile tests, dog-bone shaped lamellae 280–330 nm thick and ~ 2.5 µm long were used as objects of study. The lamellae were manufactured using the focused ion beam technology from the metal–diamond interface of diamond-containing composite material with a single-phase binder made of Fe–Co–Ni alloy. The experimentally determined bonding strength was 110 MPa.