Affiliation:
1. Boreskov Institute of Catalysis SB RAS
2. SRF “SKIF”, Boreskov Institute of Catalysis SB RAS
Abstract
Using high-resolution X-ray diffraction and synchrotron radiation, as well as and scanning electron microscopy, it has been shown that the observed high reactivity of commercial aluminum alloys activated with the Ga–In eutectic is associated with the formation of the Al–Ga–In eutectic along grain boundaries in the entire material volume. The loss of material activity during storage under atmospheric conditions is due to the oxidation of the eutectic components. Activation with pure gallium leads to formation of AlGax solid solution, which has low activity in the reaction with water under neutral pH.
Publisher
The Russian Academy of Sciences